Products
34Cr4 Steel - Nr.1.7033 34CrS4 - Nr.1.7037
What Is 34Cr4/34CrS4 Steel?
34Cr4/34CrS4 Steel: References and Comparable Standards
Standard Reference: EN ISO 683-2: 2018 (Hot-rolled products) | EN 10277: 2018 (Bright products)
| Region | Standard | Grade | Werkstoff No. |
|---|---|---|---|
| Europe | EN 10083-3: 2006 EN 10277-5: 2008 |
34Cr4 | 1.7033 |
| Italy | (UNI 7845-78) | - | - |
| Germany | (DIN 17200-86) | 34Cr4 | 1.7033 |
| France | (NF A 35-552-86) | 32C4 | - |
| UK | (BS 970 pt.3-96) | - | - |
| USA | ASTM A 29 | 5135 | - |
Europe
StandardEN 10083-3: 2006
EN 10277-5: 2008
Grade34Cr4
Werkstoff No.1.7033
Italy
Standard(UNI 7845-78)
Grade-
Werkstoff No.-
Germany
Standard(DIN 17200-86)
Grade34Cr4
Werkstoff No.1.7033
France
Standard(NF A 35-552-86)
Grade32C4
Werkstoff No.-
UK
Standard(BS 970 pt.3-96)
Grade-
Werkstoff No.-
USA
StandardASTM A 29
Grade5135
Werkstoff No.-
34Cr4/34CrS4 Steel: Chemical Composition (Cast Analysis) (%)
34Cr4/34CrS4 Steel: Mechanical Properties - As Rolled Condition
| Size (mm) |
Treated to improve shearability (+S) |
Soft annealing (+A) |
Quenched and tempered (+QT) |
||||
|---|---|---|---|---|---|---|---|
| Maximum HardnessHB | Maximum HardnessHB | Yield StrengthRp0.2 (MPa) min | Tensile StrengthRm (MPa) | ElongationA5 (%) min | Reduction of AreaZ (%) min | Notched Impact StrengthKV (J) min | |
| d≤16 | Treated to improve shearability (+S)255 | Soft annealing (+A)223 | Quenched and tempered (+QT)700 | Quenched and tempered (+QT)900-1100 | Quenched and tempered (+QT)12 | Quenched and tempered (+QT)35 | Quenched and tempered (+QT)- |
| 16<d≤40 | Treated to improve shearability (+S)255 | Soft annealing (+A)223 | Quenched and tempered (+QT)590 | Quenched and tempered (+QT)800-950 | Quenched and tempered (+QT)14 | Quenched and tempered (+QT)40 | Quenched and tempered (+QT)40 |
| 40<d≤100 | Treated to improve shearability (+S)255 | Soft annealing (+A)223 | Quenched and tempered (+QT)460 | Quenched and tempered (+QT)700-850 | Quenched and tempered (+QT)15 | Quenched and tempered (+QT)45 | Quenched and tempered (+QT)40 |
34Cr4/34CrS4 Steel: Mechanical Properties – Bright Steel
| Size (mm) |
as Rolled+Turned (+A+SH) |
Quenched+Tempered+Turned (+QT+SH)* |
Quenched+Tempered+Cold Drawn (+QT+C) |
as Rolled+Cold Drawn (+A+C) |
||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Maximum HardnessHB | Yield StrengthRp0.2 (MPa) min | Tensile StrengthRm (MPa) | ElongationA5 (%) min | Notched Impact StrengthKV (J) min | Yield StrengthRp0.2 (MPa) min | Tensile StrengthRm (MPa) | ElongationA5 (%) min | Maximum HardnessHB | Maximum HardnessHB | Maximum HardnessHB | ||
| 5≤d≤10 | as Rolled+Turned (+A+SH)- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Cold Drawn (+QT+C)700 | Quenched+Tempered+Cold Drawn (+QT+C)900-1100 | Quenched+Tempered+Cold Drawn (+QT+C)8 | as Rolled+Cold Drawn (+A+C)285 | |||
| 10<d≤16 | as Rolled+Turned (+A+SH)- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Turned (+QT+SH)*- | Quenched+Tempered+Cold Drawn (+QT+C)700 | Quenched+Tempered+Cold Drawn (+QT+C)900-1100 | Quenched+Tempered+Cold Drawn (+QT+C)9 | as Rolled+Cold Drawn (+A+C)275 | |||
| 16<d≤40 | as Rolled+Turned (+A+SH)223 | Quenched+Tempered+Turned (+QT+SH)*590 | Quenched+Tempered+Turned (+QT+SH)*800-950 | Quenched+Tempered+Turned (+QT+SH)*14 | Quenched+Tempered+Turned (+QT+SH)*40 | Quenched+Tempered+Cold Drawn (+QT+C)580 | Quenched+Tempered+Cold Drawn (+QT+C)800-1000 | Quenched+Tempered+Cold Drawn (+QT+C)9 | as Rolled+Cold Drawn (+A+C)270 | |||
| 40<d≤63 | as Rolled+Turned (+A+SH)223 | Quenched+Tempered+Turned (+QT+SH)*460 | Quenched+Tempered+Turned (+QT+SH)*700-850 | Quenched+Tempered+Turned (+QT+SH)*15 | Quenched+Tempered+Turned (+QT+SH)*40 | Quenched+Tempered+Cold Drawn (+QT+C)510 | Quenched+Tempered+Cold Drawn (+QT+C)700-900 | Quenched+Tempered+Cold Drawn (+QT+C)10 | as Rolled+Cold Drawn (+A+C)265 | |||
| 63<d≤100 | as Rolled+Turned (+A+SH)223 | Quenched+Tempered+Turned (+QT+SH)*460 | Quenched+Tempered+Turned (+QT+SH)*700-850 | Quenched+Tempered+Turned (+QT+SH)*15 | Quenched+Tempered+Turned (+QT+SH)*40 | Quenched+Tempered+Cold Drawn (+QT+C)480 | Quenched+Tempered+Cold Drawn (+QT+C)700-900 | Quenched+Tempered+Cold Drawn (+QT+C)11 | as Rolled+Cold Drawn (+A+C)265 | |||
| *This values are valid also for Cold Drawn - Quenched + Tempered Condition (+C +QT). Note: For size <5 mm the mechanical properties may be agreed at the time of enquiry and order. |
||||||||||||
34Cr4/34CrS4 Steel: Working Temperatures Recommended
| Operation | Temperature |
|---|---|
| Hot forgings deformation | 850-1150 °C |
| Isothermal annealing | 850-880-->675 °C |
| Soft annealing | 680-720 °C |
| Quenching in oil | 840-870 °C |
| Tempering | 540-660 °C |
34Cr4/34CrS4 Steel: Hardness Limits (Jominy Test)
| Limits of range | Hardness HRC at a distance from quenched end of test pieces (mm) | |||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 1,5 | 3 | 5 | 7 | 9 | 11 | 13 | 15 | 20 | 25 | 30 | 35 | 40 | 45 | 50 | ||
| +H | Max | 57 | 57 | 56 | 54 | 52 | 49 | 46 | 44 | 39 | 37 | 35 | 34 | 33 | 32 | 31 |
| Min | 49 | 48 | 45 | 41 | 35 | 32 | 29 | 27 | 23 | 21 | 20 | - | - | - | - | |
| +HH | Max | 57 | 57 | 56 | 54 | 52 | 49 | 46 | 44 | 39 | 37 | 35 | 34 | 33 | 32 | 31 |
| Min | 52 | 51 | 49 | 45 | 41 | 38 | 35 | 33 | 28 | 26 | 25 | 24 | 23 | 22 | 21 | |
| +HL | Max | 54 | 54 | 52 | 50 | 46 | 43 | 40 | 38 | 34 | 32 | 30 | 29 | 28 | 27 | 26 |
| Min | 49 | 48 | 45 | 41 | 35 | 32 | 29 | 27 | 23 | 21 | 20 | - | - | - | - | |